Abstract
The purification procedure of the LiY0.5Er0.5F4 compound for Bridgman-Stockbarger and Czochralski single crystal growth has been investigated. Yttrium and rare-earth oxyfluorides were found to form during hydrofluoric heat-treatment of the starting fluoride mixture. Optically clear single crystals of purified LiY0.5Er0.5F4 were grown by both Bridgman-Stockbarger and Czochralski methods. The stoichiometry was investigated by magnetic susceptibility measurements and the Er content in the single crystals grown by both Bridgman-Stockbarger and Czochralski methods were found to fit stoichiometry within the measurement error. No free (OH)- ions were found by infrared absorption spectroscopy.
Original language | English |
---|---|
Pages (from-to) | 381-388 |
Number of pages | 8 |
Journal | Materials Research Bulletin |
Volume | 16 |
Issue number | 4 |
DOIs | |
State | Published - Apr 1981 |